| Room temperature impact toughness of Ti-3Al-2.5V(Grade 9) Rods | ||||
| Form | d or δ/mm | State | Sampling direction | αku/kJ·m-2 |
| Rolling rods | 20 | annealing | L | 1245 |
| Forged rods | 17 | annealing | L | 814 |
| Properties of Ti-3Al-2.5V(Grade 9) Rods | |||||||||
| Form | d or δ/mm | State | Sampling direction | Room temperature | |||||
| σb/MPa | σp0.2/MPa | δ50/% | ψ5/% | ψ/% | αku/kJ·m-2 | ||||
| Rods | 8~50 | annealing | L | ≥620 | ≥518 | - | 15 | 30 | ≥500 |
| Tensile Properties of Ti-3Al-2.5V(Grade 9) Rods | |||||||||
| Form | d or δ/mm | State | Sampling direction | θ/℃ | σb/MPa | σp0.2/MPa | σ8/MPa | δ5/% | ψ/% |
| Rods | 10~25 | annealing | L | 20 | 691 | 565 | - | 18 | 41 |
| Room temperature notched tensile properties of Ti-3Al-2.5V(Grade 9) Rods | ||||||||
| Form | d or δ/mm | Processing methods | State | Sampling direction | θ/℃ | Kt | σbH/MPa | σbH/σb |
| Rods | 20 | Hot rolled | 750℃, 1h, air cooling | L | 20 | 2 | 998 | 1.53 |
| 3 | 1047 | 1.61 | ||||||
| 5 | 1041 | 1.6 | ||||||
| 12 | Cold swaging | 750℃, 1h, air cooling | L | 20 | 3 | 1069 | 1.58 | |
| Tensile properties of annealed Ti-3Al-2.5V(Grade 9) Rods specimens after thermal exposure at room temperature | |||||
| Heat exposure conditions | Rods d/mm | ||||
| 700℃, 30min, air cooling | |||||
| 20 | |||||
| θ/℃ | t/h | σb/MPa | σp0.2/MPa | δ5/% | ψ/% |
| Not exposed | 652 | 604 | 20.7 | 59.7 | |
| 400 | 500 | 658 | 612 | 23 | 60.8 |
| 1000 | 646 | 634 | 21 | 58.3 | |
| 1500 | 652 | 629 | 20 | 58.2 | |
| 2000 | - | - | - | - | |
| 470 | 400 | 652 | 628 | 22.5 | 59.8 |
| Rotating bending fatigue limit of Ti-3Al-2.5V(Grade 9) Rods at room temperature | |||||||||
| Form | d or δ/mm | State | Sampling direction | σb/MPa | σp0.2/MPa | Kt | R | N/circle | σD/MPa |
| Rods | 17 | 750℃, 1h, air cooling | L | 691 | 584 | 1 | -1 | 107 | 343 |
| 3 | -1 | 107 | 176 | ||||||
Shear modulus
The room temperature shear elastic modulus of annealed rod G=39.6GPa